Tensile Properties of 9% Nickel Steel at Elevated Temperatures
Although the 9% nickel alloy steel is not utilized normally for elevated temperature service, specific requirements allow pressure vessels to be cycled from moderately elevated temperatures to subzero temperature. A few experimental short time elevated-temperature tensile data for both NNT & QT 9% nickel steel plates are presented in below tables (*Temp.: test temperature; *THK.: plate thickness; *HT: heat treatment type; *T.S: tensile strength; *Y.S: yield strength @ 0.2% offset; *EL.: elongation 1 inch; *RA.: reduction of area).
*Temp. °F | *THK. inch | *HT | *T.S, ksi | *Y.S, ksi | *EL. % | *RA. % |
---|---|---|---|---|---|---|
Room | 1/2 | QT | 110 | 93 | 25 | 74 |
250 | 1/2 | QT | 101 | 91 | 23 | 73 |
450 | 1/2 | QT | 101 | 90 | 23 | 73 |
650 | 1/2 | QT | 95 | 82 | 31 | 78 |
850 | 1/2 | QT | 76 | 68 | 26 | 79 |
*Temp. °F | *THK. inch | *HT | *T.S, ksi | *Y.S, ksi | *EL. % | *RA. % |
---|---|---|---|---|---|---|
Room | 1/2 | NNT | 110 | 88 | 26 | 71 |
250 | 1/2 | NNT | 100 | 77 | 24 | 71 |
450 | 1/2 | NNT | 102 | 76 | 26 | 69 |
650 | 1/2 | NNT | 91 | 70 | 30 | 77 |
850 | 1/2 | NNT | 70 | 60 | 30 | 81 |
*Temp. °F | *THK. inch | *HT | *T.S, ksi | *Y.S, ksi | *EL. % | *RA. % |
---|---|---|---|---|---|---|
Room | 2 | QT | 109 | 100 | 25 | 72 |
250 | 2 | QT | 102 | 91 | 23 | 73 |
450 | 2 | QT | 101 | 88 | 22 | 69 |
650 | 2 | QT | 96 | 83 | 29 | 77 |
850 | 2 | QT | 76 | 70 | 26 | 82 |
*Temp. °F | *THK. inch | *HT | *T.S, ksi | *Y.S, ksi | *EL. % | *RA. % |
---|---|---|---|---|---|---|
Room | 2 | QT | 109 | 100 | 25 | 72 |
250 | 2 | QT | 102 | 91 | 23 | 73 |
450 | 2 | QT | 101 | 88 | 22 | 69 |
650 | 2 | QT | 96 | 83 | 29 | 77 |
850 | 2 | QT | 76 | 70 | 26 | 82 |